Abstract

ISO 28706-2:2017 specifies a test method for the determination of the resistance of flat surfaces of vitreous and porcelain enamels to boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours. This method allows the determination of the resistance of vitreous and porcelain enamels to the liquid and vapour phases of the corrosive medium simultaneously.

Status
Not Published
Current Stage
5020 - FDIS ballot initiated: 2 months. Proof sent to secretariat
Start Date
11-Nov-2026
Completion Date
14-Nov-2026

Buy Documents

Draft

ISO/PRF 28706-2 - Vitreous and porcelain enamels — Determination of resistance to chemical corrosion — Part 2: Determination of resistance to chemical corrosion by boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours

Release Date:11-Nov-2026
English language (17 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/PRF 28706-2 - Vitreous and porcelain enamels — Determination of resistance to chemical corrosion — Part 2: Determination of resistance to chemical corrosion by boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours

Release Date:11-Nov-2026
English language (17 pages)
sale 15% off
sale 15% off

Relations

Effective Date
12-Feb-2026
Effective Date
10-Aug-2024

Buy Documents

Draft

ISO/PRF 28706-2 - Vitreous and porcelain enamels — Determination of resistance to chemical corrosion — Part 2: Determination of resistance to chemical corrosion by boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours

Release Date:11-Nov-2026
English language (17 pages)
sale 15% off
sale 15% off
Draft

REDLINE ISO/PRF 28706-2 - Vitreous and porcelain enamels — Determination of resistance to chemical corrosion — Part 2: Determination of resistance to chemical corrosion by boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours

Release Date:11-Nov-2026
English language (17 pages)
sale 15% off
sale 15% off

Get Certified

Connect with accredited certification bodies for this standard

DVS-ZERT GmbH

German welding certification society.

DAKKS Germany Verified

CARES (UK Certification Authority for Reinforcing Steels)

UK certification for reinforcing steels and construction.

UKAS United Kingdom Verified

EWF/IIW (European/International Welding Federation)

International welding personnel certification.

BELAC Belgium Verified

Sponsored listings

Frequently Asked Questions

ISO/PRF 28706-2 is a draft published by the International Organization for Standardization (ISO). Its full title is "Vitreous and porcelain enamels — Determination of resistance to chemical corrosion — Part 2: Determination of resistance to chemical corrosion by boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours". This standard covers: ISO 28706-2:2017 specifies a test method for the determination of the resistance of flat surfaces of vitreous and porcelain enamels to boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours. This method allows the determination of the resistance of vitreous and porcelain enamels to the liquid and vapour phases of the corrosive medium simultaneously.

ISO 28706-2:2017 specifies a test method for the determination of the resistance of flat surfaces of vitreous and porcelain enamels to boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours. This method allows the determination of the resistance of vitreous and porcelain enamels to the liquid and vapour phases of the corrosive medium simultaneously.

ISO/PRF 28706-2 is classified under the following ICS (International Classification for Standards) categories: 25.220.50 - Enamels. The ICS classification helps identify the subject area and facilitates finding related standards.

ISO/PRF 28706-2 has the following relationships with other standards: It is inter standard links to prEN ISO 28706-2, ISO 28706-2:2017. Understanding these relationships helps ensure you are using the most current and applicable version of the standard.

ISO/PRF 28706-2 is available in PDF format for immediate download after purchase. The document can be added to your cart and obtained through the secure checkout process. Digital delivery ensures instant access to the complete standard document.

Standards Content (Sample)


International
Standard
ISO 28706-2
Third edition
Vitreous and porcelain enamels —
2027-01
Determination of resistance to
chemical corrosion —
Part 2:
Determination of resistance to
chemical corrosion by boiling acids,
boiling neutral liquids, alkaline
liquids and/or their vapours
Émaux vitrifiés — Détermination de la résistance à la corrosion
chimique —
Partie 2: Détermination de la résistance à la corrosion chimique
par des acides bouillants, des liquides neutres bouillants, ou des
liquides alcalins et/ou leurs vapeurs
PROOF/ÉPREUVE
Reference number
ISO 28706-2:2027(en) © ISO 2027

ISO 28706-2:2027(en)
© ISO 2027
All rights reserved.
This ISO publication is protected by copyright and is owned by ISO and/or its licensors.
The content of this ISO publication is provided under licence, not sold. Use is subject to the applicable licence terms issued by ISO,
an ISO member body, or an authorized third-party distributor.
Except as required for implementation or expressly permitted by a separate licence, no part of this ISO publication may be
reproduced, distributed, modified, used, or made available in any form or by any means - electronic or mechanical, including
photocopying, scanning, recording, or posting on internal or external digital platforms.
Any use beyond the scope of the granted rights is prohibited and may result in legal action.
ISO copyright office
CP 401 • CH-1214 Vernier, Geneva
Phone: +41 22 749 01 11
Email: copyright@iso.org
Website: www.iso.org
Published in Switzerland
PROOF/ÉPREUVE
ii
ISO 28706-2:2027(en)
Contents Page
Foreword .v
Introduction .vi
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 1
4 Principle . 2
5 Reagents . 2
6 Apparatus and materials . 3
6.1 Test apparatus.3
6.1.1 General .3
6.1.2 Apparatus . .6
6.2 Test materials .8
7 Packing rings . 8
7.1 General .8
7.2 Packing A .8
7.3 Packing B .8
8 Test specimens . 9
9 Procedure . 9
10 Expression of results . 9
10.1 Total loss in mass per unit area .9
10.2 Corrosion rate .10
11 Boiling citric acid . 10
11.1 General .10
11.2 Test solution .10
11.3 Duration of the test .11
11.4 Test report .11
12 Boiling sulfuric acid .11
12.1 General .11
12.2 Test solution .11
12.3 Duration of the test .11
12.4 Test report .11
13 Boiling hydrochloric acid .12
13.1 General . 12
13.2 Test solution . 12
13.3 Duration of the test . 12
13.4 Test report . 12
14 Boiling distilled or demineralized water .13
14.1 General . 13
14.2 Test solution . 13
14.3 Duration of the test . 13
14.4 Test report . 13
15 Standard detergent solution . 14
15.1 General .14
15.2 Test solution .14
15.3 Test temperature .14
15.4 Duration of the test .14
15.5 Test report .14
16 Other test solutions and/or conditions .15
PROOF/ÉPREUVE
iii
ISO 28706-2:2027(en)
16.1 General . 15
16.2 Test solution . 15
16.3 Duration of the test . 15
16.4 Test report . 15
Bibliography . 17
PROOF/ÉPREUVE
iv
ISO 28706-2:2027(en)
Foreword
ISO (the International Organization for Standardization) is a worldwide federation of national standards
bodies (ISO member bodies). The work of preparing International Standards is normally carried out through
ISO technical committees. Each member body interested in a subject for which a technical committee
has been established has the right to be represented on that committee. International organizations,
governmental and non-governmental, in liaison with ISO, also take part in the work. ISO collaborates closely
with the International Electrotechnical Commission (IEC) on all matters of electrotechnical standardization.
The procedures used to develop this document and those intended for its further maintenance are described
in the ISO/IEC Directives, Part 1. In particular, the different approval criteria needed for the different types
of ISO document should be noted. This document was drafted in accordance with the editorial rules of the
ISO/IEC Directives, Part 2 (see www.iso.org/directives).
ISO draws attention to the possibility that the implementation of this document may involve the use of (a)
patent(s). ISO takes no position concerning the evidence, validity or applicability of any claimed patent
rights in respect thereof. As of the date of publication of this document, ISO had not received notice of (a)
patent(s) which may be required to implement this document. However, implementers are cautioned that
this may not represent the latest information, which may be obtained from the patent database available at
www.iso.org/patents. ISO shall not be held responsible for identifying any or all such patent rights.
Any trade name used in this document is information given for the convenience of users and does not
constitute an endorsement.
For an explanation of the voluntary nature of standards, the meaning of ISO specific terms and expressions
related to conformity assessment, as well as information about ISO's adherence to the World Trade
Organization (WTO) principles in the Technical Barriers to Trade (TBT), see www.iso.org/iso/foreword.html.
This document was prepared by Technical Committee ISO/TC 107, Metallic and other inorganic coatings,
in collaboration with the European Committee for Standardization (CEN) Technical Committee CEN/TC
262, Metallic and other inorganic coatings, including for corrosion protection and corrosion testing of metals
and alloys, in accordance with the Agreement on technical cooperation between ISO and CEN (Vienna
Agreement).
This third edition cancels and replaces the second edition (ISO 28706-2:2017), which has been technically
revised.
The main changes are as follows:
— The simmering aid part of the test apparatus has been removed as it is not required for this test.
— The testing procedure has been updated to include the requirement for tests to be carried out in a
temperature-controlled environment and to define a time for emptying the test cylinder.
A list of all parts in the ISO 28706 series can be found on the ISO website.
Any feedback or questions on this document should be directed to the user’s national standards body. A
complete listing of these bodies can be found at www.iso.org/members.html.
PROOF/ÉPREUVE
v
ISO 28706-2:2027(en)
Introduction
Corrosion of vitreous and porcelain enamels by aqueous solutions is a dissolution process. The main
component of the enamel, SiO , forms a three-dimensional silica network. After hydrolysis, it decomposes
and forms silicic acid or silicates. These are released into the attacking medium. Other components, mainly
metal oxides, are hydrolysed as well and form the corresponding hydrated metal ions or hydroxides. All
corrosion products are soluble in the attacking medium. The whole process results in a loss in mass per unit
area.
For some aqueous solutions, the attack on the enamel proceeds linearly during the corrosion time. For other
aqueous solutions, the attack on the enamel proceeds in a logarithmic manner during the corrosion time.
Only for the first series of solutions can a scientifically exact rate of loss in mass per unit area (g/m ·h) be
calculated as well as a corrosion rate (millimetres per year).
The most important parameters influencing aqueous corrosion of the enamel are the enamel quality, the
temperature and the pH value. Inhibition effects resulting from the limited solubility of silica can also
contribute. The following list describes different types of enamel attack for different corrosion conditions.
a) In aqueous alkali solutions such as 0,1 mol/l NaOH (see ISO 28706-4:2026, Clause 10), the silica network
of the enamel is considerably attacked at 80 °C. Silicates and most of the other hydrolysed components
are soluble in the alkali. Attack proceeds linearly during regular test times. Therefore, test results
are expressed in terms of a rate of loss in mass per unit area (mass loss per unit area and time) and a
corrosion rate (millimetres per year).
b) At room temperature, in weak aqueous acids such as citric acid (see ISO 28706-1:2008, Clause 9) and
in stronger acids such as sulfuric acid (see ISO 28706-1:2008, Clause 10), there is only minor attack on
the silica network of the enamel. Other constituents are leached to some extent from the surface. Highly
resistant enamels will show no visual change after exposure. On less resistant enamels, some staining
or surface roughening will occur.
c) In boiling aqueous acids (as described in this document), the silica network of the enamel is being
attacked and silica as well as the other enamel components are released into solution. However, the
solubility of silica in acids is low. Soon, the attacking solutions will become saturated with dissolved
silica and will then only leach the surface. The acid attack is inhibited and the rate of corrosion drops
markedly.
NOTE The glass test equipment also releases silica by acid attack and contributes to the inhibition of the
corrosion.
Inhibition is effectively prevented in vapour phase tests. The condensate formed on the test specimen is
free of any dissolved enamel constituents.
Examples of enamel corrosion proceeding in a logarithmic manner [see 1)] and linearly [see 2)] are as
follows:
1) Boiling citric acid (see Clause 11) and boiling 30 % sulfuric acid (see Clause 12).
Since only minute amounts of these acids are found in their vapours, the test is restricted to the
liquid phase. The attack is influenced by inhibition effects and corrosion depends on the time of
exposure. Therefore, test results are expressed in terms of loss in mass per unit area; no rate of loss
in mass per unit area is calculated.
2) Boiling 20 % hydrochloric acid (see Clause 13).
Since this is an azeotropic boiling acid, its concentration in the liquid and the vapour phase are
identical, and liquid phase testing is not required. Vigorous boiling supplies an uninhibited
condensate and the attack proceeds linearly with time of exposure. Therefore, test results are only
expressed in terms of rate of loss in mass per unit area (mass loss per unit area and time) and the
corrosion rate (millimetres per year).
PROOF/ÉPREUVE
vi
ISO 28706-2:2027(en)
d) At high temperatures, with tests in the liquid phase under autoclave conditions (see ISO 28706-5),
aqueous acid attack is severe. To avoid inhibition, the test time is restricted to 24 h and the ratio of
attacking acid to attacked enamel surface is chosen so that it is comparatively high (similar to that in a
chemical reaction vessel). In addition, only low-silica water is used for the preparation of test solutions.
Under these conditions, attack will proceed linearly with time of exposure. Therefore, test results with
20 % hydrochloric acid (see ISO 28706-5:2010, Clause 8), artificial test solutions (see ISO 28706-5:2010,
Clause 10) or process fluids (see ISO 28706-5:2010, Clause 11) are also expressed in terms of a rate of
loss in mass per unit area (loss in mass per unit area and time).
e) In boiling water (see Clause 14), the silica network is fairly stable. The enamel surface is leached and
silica is dissolved only to a small extent. This type of attack is clearly represented by the vapour phase
attack. In the liquid phase, some inhibition can be observed with highly resistant enamels. However, if
the enamel being tested is weak, leached alkali from the enamel can raise pH values to alkaline levels,
thus increasing the attack by the liquid phase. Both liquid and vapour phase testing can give valuable
information.
f) Since it is possible that the attack is not linear, the results are expressed only in terms of loss in mass per
unit area and the test time should be indicated.
g) For standard detergent solution (see ISO 28706-3:2017, Clause 9), it will not be certain whether the
linear part of the corrosion curve will be reached during testing for 24 h or 168 h. Calculation of the
corrosion rate is therefore not included in the test report.
h) For other acids (see Clause 15) and other alkaline solutions (see ISO 28706-3:2017, Clause 10 and
ISO 28706-4:2016, Clause 11), it will also not be known if a linear corrosion rate will be reached during
the test period. Calculation of the corrosion rate is therefore not included in the test reports of those
parts of this document.
For vitreous enamels fired at temperatures below 700 °C, the test parameters (media, temperatures and
times) of this document are not appropriate. For such enamels, for example aluminium enamels, other
media, temperatures and/or times should be used. This can be done following the procedures described in
ISO 28706-1, this document, ISO 28706-3 and ISO 28706-4.
PROOF/ÉPREUVE
vii
International Standard ISO 28706-2:2027(en)
Vitreous and porcelain enamels — Determination of
resistance to chemical corrosion —
Part 2:
Determination of resistance to chemical corrosion by boiling
acids, boiling neutral liquids, alkaline liquids and/or their
vapours
WARNING — This document calls for the use of substances and/or procedures that can be injurious
to health if adequate safety measures are not taken. This document does not address any health
hazards, safety or environmental matters associated with its use. Is it the responsibility of the user
of this document to establish appropriate health, safety and environmentally acceptable practices
and take suitable actions for any national and international regulations.
1 Scope
This document specifies a test method for the determination of the resistance of flat surfaces of vitreous and
porcelain enamels to boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours.
This method allows the determination of the resistance of vitreous and porcelain enamels to the liquid and
vapour phases of the corrosive medium simultaneously.
2 Normative references
The following documents are referred to in the text in such a way that some or all of their content constitutes
requirements of this document. For dated references, only the edition cited applies. For undated references,
the latest edition of the referenced document (including any amendments) applies.
ISO 48, Rubber, vulcanized or thermoplastic — Determination of hardness (hardness between 10 IRHD and 100
IRHD)
ISO 649-1, Laboratory glassware — Density hydrometers for general purposes — Part 1: Specification
ISO 718, Laboratory glassware — Thermal shock and thermal shock endurance — Test methods
ISO 3585, Borosilicate glass 3.3 — Properties
ISO 3696, Water for analytical laboratory use — Specification and test methods
ISO 4788, Laboratory glassware — Graduated measuring cylinders
ISO 4799, Laboratory glassware — Condensers
ISO 28764, Vitreous and porcelain enamels — Production of specimens for testing enamels on sheet steel, sheet
aluminium and cast iron
3 Terms and definitions
No terms and definitions are listed in this document.
PROOF/ÉPREUVE
ISO 28706-2:2027(en)
ISO and IEC maintain terminology databases for use in standardization at the following addresses:
— ISO Online browsing platform: available at https:// www .iso .org/ obp
— IEC Electropedia: available at https:// www .electropedia .org/
4 Principle
A set of similarly enamelled test specimens is placed in the liquid zone and/or in the vapour zone of the test
apparatus, as required, and exposed to a
...


Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
Style Definition
...
ISO /TC 107
Style Definition
...
Style Definition
...
Secretariat: KATS
Style Definition
...
Style Definition
Date: 2026-11 August 2026-10 .
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Vitreous and porcelain enamels — Determination of resistance to
Style Definition
...
chemical corrosion —
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Part 2:
Style Definition
...
Determination of resistance to chemical corrosion by boiling
Style Definition
...
acids, boiling neutral liquids, alkaline liquids and/or their
Style Definition
...
vapours
Style Definition
...
Style Definition
...
Émaux vitrifiés — Détermination de la résistance à la corrosion chimique —
Style Definition
...
Style Definition
...
Partie 2: Détermination de la résistance à la corrosion chimique par des acides bouillants, des liquides
Style Definition
neutres bouillants, ou des liquides alcalins et/ou leurs vapeurs
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
Style Definition
...
l fi i i
© PROOF
Formatted: HeaderCentered
© ISO 2026
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
All rights reserved. Unless otherwise specified,
Formatted: Adjust space between Latin and Asian text,
This ISO publication is protected by copyright and is owned by ISO and/or its licensors.
Adjust space between Asian text and numbers
The content of this ISO publication is provided under licence, not sold. Use is subject to the applicable licence terms issued
Formatted: Right: 1.5 cm, Gutter: 0 cm, Header distance
by ISO, an ISO member body, or an authorized third-party distributor.
from edge: 1.27 cm, Footer distance from edge: 0.5 cm
Except as required in the context of its for implementation or expressly permitted by a separate licence, no part of this
ISO publication may be reproduced or utilized otherwise, distributed, modified, used, or made available in any form or
by any means, – electronic or mechanical, including photocopying, scanning, recording, or posting on internal or external
digital platforms.
Any use beyond the internet or an intranet, without prior written permission. Permission can be requested from either Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers
ISO at the address below or ISO’s member body in the countryscope of the requestergranted rights is prohibited and may
result in legal action.
ISO copyright office
CP 401 • Ch. de Blandonnet 8
CH-1214 Vernier, Geneva
Formatted: zzCopyright address, Adjust space between Latin
and Asian text, Adjust space between Asian text and numbers
Phone: + 41 22 749 01 11
Email: copyright@iso.org
Website: www.iso.orgwww.iso.org
Published in Switzerland
Formatted: Font: 10 pt, Not Bold
Formatted: Font: 10 pt, Not Bold
Formatted: Font: 10 pt, Not Bold
Formatted: FooterCentered
© ISO 2025 2026 – All rights reserved
ii
Formatted: Font: 11 pt, Font color: Auto
Formatted: Font: Bold
Contents Page Formatted: HeaderCentered, Left
Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers, Tab stops: Not
Foreword . vi
at 0.71 cm + 17.2 cm
Introduction . vii
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 2
4 Principle . 2
5 Reagents . 2
6 Apparatus and materials . 3
6.1 Test apparatus . 3
6.2 Test materials . 13
7 Packing rings . 13
7.1 General . 13
7.2 Packing A . 13
7.3 Packing B . 14
8 Test specimens . 14
9 Procedure . 14
10 Expression of results . 15
10.1 Total loss in mass per unit area . 15
10.2 Corrosion rate . 15
11 Boiling citric acid . 16
11.1 General . 16
11.2 Test solution . 16
11.3 Duration of the test . 16
11.4 Test report . 16
12 Boiling sulfuric acid . 16
12.1 General . 16
12.2 Test solution . 17
12.3 Duration of the test . 17
12.4 Test report . 17
13 Boiling hydrochloric acid . 17
13.1 General . 17
13.2 Test solution . 17
13.3 Duration of the test . 17
13.4 Test report . 18
14 Boiling distilled or demineralized water . 18
14.1 General . 18
14.2 Test solution . 18
14.3 Duration of the test . 18
14.4 Test report . 19
Formatted: Font: 10 pt
15 Standard detergent solution . 19
Formatted: Font: 10 pt
15.1 General . 19
Formatted: Font: 10 pt
15.2 Test solution . 19
15.3 Test temperature . 20
Formatted: FooterCentered, Left, Space Before: 0 pt, Tab
stops: Not at 17.2 cm
15.4 Duration of the test . 20
Formatted: Font: 11 pt
© ISO 2026 – All rights reserved
iii
Formatted: HeaderCentered
15.5 Test report . 20
16 Other test solutions and/or conditions . 20
16.1 General . 20
16.2 Test solution . 21
16.3 Duration of the test . 21
16.4 Test report . 21
Bibliography . 22

Foreword . v
Introduction . vi
1 Scope . 1
2 Normative references . 1
3 Terms and definitions . 2
4 Principle . 2
5 Reagents . 2
6 Apparatus and materials . 3
6.1 Test apparatus . 3
6.1.1 General . 3
6.1.2 Apparatus . 6
6.2 Test materials . 8
7 Packing rings . 9
7.1 General . 9
7.2 Packing A . 9
7.3 Packing B . 9
8 Test specimens . 9
9 Procedure . 9
10 Expression of results . 10
10.1 Total loss in mass per unit area . 10
10.2 Corrosion rate . 10
11 Boiling citric acid . 11
11.1 General . 11
11.2 Test solution . 11
11.3 Duration of the test . 11
11.4 Test report . 11
12 Boiling sulfuric acid . 12
12.1 General . 12
12.2 Test solution . 12
12.3 Duration of the test . 12
12.4 Test report . 12
13 Boiling hydrochloric acid . 13
13.1 General . 13
13.2 Test solution . 13
Formatted: Font: 10 pt, Not Bold
13.3 Duration of the test . 13
13.4 Test report . 13
Formatted: Font: 10 pt, Not Bold
Formatted: Font: 10 pt, Not Bold
14 Boiling distilled or demineralized water . 14
Formatted: FooterCentered
© ISO 2025 2026 – All rights reserved
iv
Formatted: Font: 11 pt, Font color: Auto
Formatted: Font: Bold
14.1 General . 14
Formatted: HeaderCentered, Left
14.2 Test solution . 14
14.3 Duration of the test . 14
14.4 Test report . 14
15 Standard detergent solution . 15
15.1 General . 15
15.2 Test solution . 15
15.3 Test temperature . 15
15.4 Duration of the test . 15
15.5 Test report . 15
16 Other test solutions and/or conditions . 16
16.1 General . 16
16.2 Test solution . 16
16.3 Duration of the test . 16
16.4 Test report . 16
Bibliography . 18

Formatted: Font: 10 pt
Formatted: Font: 10 pt
Formatted: Font: 10 pt
Formatted: FooterCentered, Left, Space Before: 0 pt, Tab
stops: Not at 17.2 cm
Formatted: Font: 11 pt
© ISO 2026 – All rights reserved
v
Formatted: HeaderCentered
Formatted: Adjust space between Latin and Asian text,
Foreword
Adjust space between Asian text and numbers
ISO (the International Organization for Standardization) is a worldwide federation of national standards
bodies (ISO member bodies). The work of preparing International Standards is normally carried out through
ISO technical committees. Each member body interested in a subject for which a technical committee has been
established has the right to be represented on that committee. International organizations, governmental and
non-governmental, in liaison with ISO, also take part in the work. ISO collaborates closely with the
International Electrotechnical Commission (IEC) on all matters of electrotechnical standardization.
The procedures used to develop this document and those intended for its further maintenance are described
in the ISO/IEC Directives, Part 1. In particular, the different approval criteria needed for the different types of
ISO document should be noted. This document was drafted in accordance with the editorial rules of the
ISO/IEC Directives, Part 2 (see www.iso.org/directives). Formatted: English (United Kingdom)
Formatted: Default Paragraph Font, English (United
Kingdom)
ISO draws attention to the possibility that the implementation of this document may involve the use of (a)
patent(s). ISO takes no position concerning the evidence, validity or applicability of any claimed patent rights
in respect thereof. As of the date of publication of this document, ISO had not received notice of (a) patent(s)
which may be required to implement this document. However, implementers are cautioned that this may not
represent the latest information, which may be obtained from the patent database available at
www.iso.org/patents.www.iso.org/patents. ISO shall not be held responsible for identifying any or all such
patent rights.
Any trade name used in this document is information given for the convenience of users and does not
constitute an endorsement.
For an explanation of the voluntary nature of standards, the meaning of ISO specific terms and expressions
related to conformity assessment, as well as information about ISO's adherence to the World Trade
Organization (WTO) principles in the Technical Barriers to Trade (TBT), see
www.iso.org/iso/foreword.htmlwww.iso.org/iso/foreword.html. Formatted: English (United Kingdom)
This document was prepared by Technical Committee ISO/TC 107, Metallic and other inorganic coatings, in
Formatted: Font: Not Italic
collaboration with the European Committee for Standardization (CEN) Technical Committee CEN/TC 262,
Formatted: Font: Not Italic
Metallic and other inorganic coatings, including for corrosion protection and corrosion testing of metals and
Formatted: Default Paragraph Font
alloys, in accordance with the Agreement on technical cooperation between ISO and CEN (Vienna Agreement).
Formatted: Default Paragraph Font
This third edition cancels and replaces the second edition (ISO 28706--2:2017), which has been technically
Formatted: Default Paragraph Font
revised.
Formatted: Default Paragraph Font
Formatted: Adjust space between Latin and Asian text,
The main changes are as follows:
Adjust space between Asian text and numbers
Formatted: Adjust space between Latin and Asian text,
— — The simmering aid part of the test apparatus has been removed as it is not required for this test.
Adjust space between Asian text and numbers, Tab stops: Not
at 0.7 cm + 1.4 cm + 2.1 cm + 2.8 cm + 3.5 cm + 4.2
— — The testing procedure has been updated to include the requirement for tests to be carried out in a cm + 4.9 cm + 5.6 cm + 6.3 cm + 7 cm
temperature-controlled environment and to define a time for emptying the test cyclinercylinder. Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
A list of all parts in the ISO 28706 series can be found on the ISO website.
Formatted: Default Paragraph Font
Formatted: Adjust space between Latin and Asian text,
Any feedback or questions on this document should be directed to the user’s national standards body. A
Adjust space between Asian text and numbers
complete listing of these bodies can be found at www.iso.org/members.htmlwww.iso.org/members.html.
Formatted: English (United Kingdom)
Formatted: English (United Kingdom)
Formatted: Font: 10 pt, Not Bold
Formatted: Font: 10 pt, Not Bold
Formatted: Font: 10 pt, Not Bold
Formatted: FooterCentered
© ISO 2025 2026 – All rights reserved
vi
Formatted: Font: 11 pt, Font color: Auto
Formatted: Font: Bold
Formatted: HeaderCentered, Left
Introduction
Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers
Corrosion of vitreous and porcelain enamels by aqueous solutions is a dissolution process. The main
component of the enamel, SiO , forms a three-dimensional silica network. After hydrolysis, it decomposes and
forms silicic acid or silicates. These are released into the attacking medium. Other components, mainly metal
oxides, are hydrolysed as well and form the corresponding hydrated metal ions or hydroxides. All corrosion
products are more or less soluble in the attacking medium. The whole process results in a loss in mass per
unit area.
For some aqueous solutions, the attack on the enamel proceeds linearly during the corrosion time. For other
aqueous solutions, the attack on the enamel proceeds in a logarithmic manner during the corrosion time. Only
for the first series of solutions can a scientifically exact rate of loss in mass per unit area (g/m ·h) be calculated
as well as a corrosion rate (millimetres per year).
The most important parameters influencing aqueous corrosion of the enamel are the enamel quality, the
temperature and the pH value. Inhibition effects resulting from the limited solubility of silica can also
contribute. The following list describes different types of enamel attack for different corrosion conditions.
a) a) In aqueous alkali solutions such as 0,1 mol/l NaOH (see ISO 28706--4:2026, Clause 10), the Formatted: Default Paragraph Font
silica network of the enamel is considerably attacked at 80 °C. Silicates and most of the other hydrolysed
Formatted: Default Paragraph Font
components are soluble in the alkali. Attack proceeds linearly during regular test times. Therefore, test
Formatted: Default Paragraph Font
results are expressed in terms of a rate of loss in mass per unit area (mass loss per unit area and time)
Formatted: Default Paragraph Font
and a corrosion rate (millimetres per year).
Formatted: Numbered + Level: 1 + Numbering Style: a, b,
c, … + Start at: 1 + Alignment: Left + Aligned at: 0 cm +
b) b) At room temperature, in weak aqueous acids such as citric acid (see ISO 28706--1:2008,
Indent at: 0 cm, Adjust space between Latin and Asian text,
Clause 9) and in stronger acids such as sulfuric acid (see ISO 28706--1:2008, Clause 10), there is only Adjust space between Asian text and numbers, Tab stops: Not
at 0.7 cm + 1.4 cm + 2.1 cm + 2.8 cm + 3.5 cm + 4.2
minor attack on the silica network of the enamel. Other constituents are leached to some extent from the
cm + 4.9 cm + 5.6 cm + 6.3 cm + 7 cm
surface. Highly resistant enamels will show no visual change after exposure. On less resistant enamels,
Formatted: Default Paragraph Font
some staining or surface roughening will occur.
Formatted: Default Paragraph Font
c) c) In boiling aqueous acids (as described in this document), the silica network of the enamel is Formatted: Default Paragraph Font
being attacked and silica as well as the other enamel components are released into solution. However, the
Formatted: Default Paragraph Font
solubility of silica in acids is low. Soon, the attacking solutions will become saturated with dissolved silica
Formatted: Default Paragraph Font
and will then only leach the surface. The acid attack is inhibited and the rate of corrosion drops markedly.
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
NOTE The glass test equipment also releases silica by acid attack and contributes to the inhibition of the
corrosion.
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
Inhibition is effectively prevented in vapour phase tests. The condensate formed on the test specimen is
Formatted: Default Paragraph Font
free of any dissolved enamel constituents.
Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers
Examples of enamel corrosion proceeding in a logarithmic manner [see 1)]1)] and linearly [see 2)]2)] are
as follows:
1) 1) Boiling citric acid (see Clause 11)Clause 11) and boiling 30 % sulfuric acid (see
Clause 12).Clause 12).
Formatted: Adjust space between Latin and Asian text,
Since only minute amounts of these acids are found in their vapours, the test is restricted to the liquid
Adjust space between Asian text and numbers
phase. The attack is influenced by inhibition effects and corrosion depends on the time of exposure.
Formatted: Font: 10 pt
Therefore, test results are expressed in terms of loss in mass per unit area; no rate of loss in mass per
unit area is calculated. Formatted: Font: 10 pt
Formatted: Font: 10 pt
2) 2) Boiling 20 % hydrochloric acid (see Clause 13).Clause 13).
Formatted: FooterCentered, Left, Space Before: 0 pt, Tab
stops: Not at 17.2 cm
Formatted: Font: 11 pt
© ISO 2026 – All rights reserved
vii
Formatted
...
Formatted
...
Formatted
Formatted
...
Formatted
...
Formatted
Since this is an azeotropic boiling acid, its concentration in the liquid and the vapour phase are
...
identical, and liquid phase testing is not required. Vigorous boiling supplies an uninhibited
Formatted
...
condensate and the attack proceeds linearly with time of exposure. Therefore, test results are only
Formatted
...
expressed in terms of rate of loss in mass per unit area (mass loss per unit area and time) and the
Formatted
...
corrosion rate (millimetres per year).
Formatted
...
Formatted
d) d) At high temperatures, with tests in the liquid phase under autoclave conditions (see
...
ISO 28706--5), aqueous acid attack is severe. To avoid inhibition, the test time is restricted to 24 h and Formatted
...
the ratio of attacking acid to attacked enamel surface is chosen so that it is comparatively high (similar to
Formatted
...
that in a chemical reaction vessel). In addition, only low-silica water is used for the preparation of test
Formatted
...
solutions. Under these conditions, attack will proceed linearly with time of exposure. Therefore, test
Formatted
...
results with 20 % hydrochloric acid (see ISO 28706--5:2010, Clause 8), artificial test solutions (see
Formatted
ISO 28706--5:2010, Clause 10) or process fluids (see ISO 28706--5:2010, Clause 11) are also expressed in .
Formatted
terms of a rate of loss in mass per unit area (loss in mass per unit area and time).
...
Formatted
...
e) e) In boiling water (see Clause 14),Clause 14), the silica network is fairly stable. The enamel
Formatted
...
surface is leached and silica is dissolved only to a small extent. This type of attack is clearly represented
Formatted
...
by the vapour phase attack. In the liquid phase, some inhibition can be observed with highly resistant
Formatted
...
enamels. However, if the enamel being tested is weak, leached alkali from the enamel can raise pH values
Formatted
to alkaline levels, thus increasing the attack by the liquid phase. Both liquid and vapour phase testing can
...
give valuable information. Formatted
...
Formatted
...
f) f) Since it is possible that the attack is not linear, the results are expressed only in terms of loss
Formatted
...
in mass per unit area and the test time should be indicated.
Formatted
...
Formatted
g) g) For standard detergent solution (see ISO 28706--3:2017, Clause 9), it will not be certain .
whether the linear part of the corrosion curve will be reached during testing for 24 h or 168 h. Calculation Formatted
...
of the corrosion rate is therefore not included in the test report.
Formatted
...
Formatted
...
h) h) For other acids (see Clause 15)Clause 15) and other alkaline solutions (see ISO 28706--3:2017,
Formatted
...
Clause 10 and ISO 28706--4:2016, Clause 11), it will also not be known if a linear corrosion rate will be
Formatted
...
reached during the test period. Calculation of the corrosion rate is therefore not included in the test
reports of those parts of this document. Formatted
...
Formatted
...
For vitreous enamels fired at temperatures below 700 °C, the test parameters (media, temperatures and
Formatted
...
times) of this document are not appropriate. For such enamels, for example aluminium enamels, other media,
Formatted
...
temperatures and/or times should be used. This can be done following the procedures described in
Formatted
...
ISO 28706--1, this document, ISO 28706--3 and ISO 28706--4.
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
Formatted
...
© ISO 2025 2026 – All rights reserved
viii
International Standard ISO 28706-2:2026(en)
Formatted: Font: Not Bold
Formatted: Header, Centered, Space After: 0 pt, Line
spacing: single
Vitreous and porcelain enamels — Determination of resistance to
chemical corrosion — Part 2: Determination of resistance to chemical
corrosion by boiling acids, boiling neutral liquids, alkaline liquids
and/or their vapours
Formatted: Right: 1.5 cm, Gutter: 0 cm, Header distance
from edge: 1.27 cm, Footer distance from edge: 0.5 cm
Vitreous and porcelain enamels — Determination of resistance to
chemical corrosion —
Part 2:
Determination of resistance to chemical corrosion by boiling acids,
boiling neutral liquids, alkaline liquids and/or their vapours
WARNING — This document calls for the use of substances and/or procedures that can be injurious to Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers
health if adequate safety measures are not taken. This document does not address any health hazards,
safety or environmental matters associated with its use. Is it the responsibility of the user of this
document to establish appropriate health, safety and environmentally acceptable practices and take
suitable actions for any national and international regulations.
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
1 Scope
Formatted: Default Paragraph Font
This document specifies a test method for the determination of the resistance of flat surfaces of vitreous and
Formatted: Adjust space between Latin and Asian text,
porcelain enamels to boiling acids, boiling neutral liquids, alkaline liquids and/or their vapours.
Adjust space between Asian text and numbers, Tab stops: Not
at 0.7 cm + 1.4 cm + 2.1 cm + 2.8 cm + 3.5 cm + 4.2
cm + 4.9 cm + 5.6 cm + 6.3 cm + 7 cm
This method allows the determination of the resistance of vitreous and porcelain enamels to the liquid and
Formatted: Default Paragraph Font
vapour phases of the corrosive medium simultaneously.
Formatted: Default Paragraph Font
2 Normative references
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
The following documents are referred to in the text in such a way that some or all of their content constitutes
Formatted: Default Paragraph Font
requirements of this document. For dated references, only the edition cited applies. For undated references,
Formatted: Default Paragraph Font
the latest edition of the referenced document (including any amendments) applies.
Formatted: Default Paragraph Font
ISO 48, Rubber, vulcanized or thermoplastic — Determination of hardness (hardness between 10 IRHD and Formatted: Default Paragraph Font
100 IRHD)
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
ISO 649--1, Laboratory glassware — Density hydrometers for general purposes — Part 1: Specification
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
ISO 718, Laboratory glassware — Thermal shock and thermal shock endurance — Test methods
Formatted: Default Paragraph Font
ISO 3585, Borosilicate glass 3.3 — Properties
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
ISO 3696, Water for analytical laboratory use — Specification and test methods
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
ISO 4788, Laboratory glassware — Graduated measuring cylinders
Formatted: Default Paragraph Font
ISO 4799, Laboratory glassware — Condensers
Formatted: Default Paragraph Font
Formatted: HeaderCentered
ISO 28764, Vitreous and porcelain enamels — Production of specimens for testing enamels on sheet steel, Formatted: Default Paragraph Font
sheet aluminium and cast iron
Formatted: Default Paragraph Font
Formatted: Default Paragraph Font
3 Terms and definitions
Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers
No terms and definitions are listed in this document.
ISO and IEC maintain terminology databases for use in standardization at the following addresses: Formatted: English (United Kingdom)
Formatted: Font: Cambria, 11 pt, English (United Kingdom)
— — ISO Online browsing platform: available at https://www.iso.org/obphttps://www.iso.org/obp
Formatted: English (United Kingdom)
Formatted: Default Paragraph Font, Font color: Auto, English
— — IEC Electropedia: available at https://www.electropedia.org/https://www.electropedia.org/
(United Kingdom)
Formatted: English (United Kingdom)
4 Principle
Formatted: Default Paragraph Font, Font color: Auto, English
(United Kingdom)
A set of similarly enamelled test specimens is placed in the liquid zone and/or in the vapour zone of the test
Formatted: Adjust space between Latin and Asian text,
apparatus, as required, and exposed to attack by a boiling acid or boiling neutral liquid, or its vapour, under
Adjust space between Asian text and numbers
specified conditions.
The same design of test apparatus and the same test principle is employed for the different liquids.
Formatted: Font: 11 pt, Not Bold
The loss in mass is determined and used to calculate the rate of loss in mass per unit area and, if necessary,
Formatted: Font: 11 pt, Not Bold
the corrosion rate.
Formatted: Adjust space between Latin and Asian text,
Adjust space between Asian text and numbers, Tab stops: Not
5 Reagents
at 0.7 cm + 1.4 cm + 2.1 cm + 2.8 cm + 3.5 cm + 4.2
cm + 4.9 cm + 5.6 cm + 6.3 cm + 7 cm
During the determination, use only reagents of recognized analytical grade, unless otherwise specified. Formatted: Font: Not Bold
Formatted: Font: 11 pt, Not Bold
5.1 5.1 Water, shall be in accordance with grade 3 of ISO 3696, i.e. distilled water or water of
Formatted: Font: Not Bold
equivalent purity.
Formatted: Font: 11 pt, Not Bold
5.2 5.2 Acetic acid solution, volume concentration 50 ml/l, for cleaning the test apparatus and test Formatted: Font: Not Bold
specimens.
Formatted: Font: 11 pt, Not Bold
Formatted: Font: Not Bold
5.3 5.3 Degreasing solvent, such as ethanol or water containing a few drops of liquid detergent,
Formatted: Font: 11 pt, Not Bold
suitable for cleaning the test apparatus and test specimens.
Formatted: Font: Not Bold
5.4 5.4 Citric acid monohydrate, (C H O ·H 0), crystalline.
6 8 7 2 Formatted: Font: 11 pt, Not Bold
Formatted: Font: Not Bold
5.5 5.5 Sulfuric acid, analytical grade, 30 % (by mass) solution, density range 1,217 g/ml to
Formatted: Font: 11 pt, Not Bold
1,220 g/ml (measured with a hydrometer; see 6.2.7).6.2.7).
Formatted: Font: Not Bold
Formatted: Font: 11 pt, Not Bold
5.6 5.6 Hydrochloric acid, analytical grade, 20 % (by mass) solution, density range 1,097 g/ml to
1,099 g/ml (measured with a hydrometer; see 6.2.7).6.2.7).
Formatted: Font: Not Bold
Formatted: Font: 11 pt, Not Bold
5.7 5.7 Sodium tripolyphosphate (Na5P3O10).
Formatted: Font: Not Bold
Formatted: Font: 11 pt, Not Bold
5.8 5.8 Sodium carbonate (Na CO ), anhydrous.
2 3
Formatted: Font: Not Bold
5.9 5.9 Sodium perborate, hydrated (NaBO ·H O ·3H O).
2 2 2 2
Formatted: Font: 11 pt, Not Bold
Formatted: Font: Not Bold
5.10 5.10 Sodium silicate, containing about 81 % (by mass) of Na SiO .
2 3
Formatted: Font: 10 pt, Not Bold
5.11 5.11 Alkylsulfonate [CH (CH ) – C(SO Na)H – (CH ) – CH ]. Formatted: Font: 10 pt, Not Bold
3 2 x 2 2 3 3
Formatted: Font: 10 pt, Not Bold
Formatted: FooterCentered
© ISO 2025 2026 – All rights reserved
Formatted: Font: 11 pt, Font color: Auto
Formatted: Font: Bold
6 Apparatus and materials
Formatted: HeaderCentered, Left
Formatted: Adjust space between Latin and Asian text,
6.1 Test apparatus
Adjust space between Asian text and numbers
Formatted: Adjust space between Latin and Asian text,
6.1.1 General
Adjust space between Asian text and numbers, Tab stops: Not
at 0.71 cm
The test apparatus (see Figure 1Figure 1 and Figure 2)Figure 2) shall consist of a cylinder (6.1.2.1;(6.1.2.1; see
Formatted: Default Paragraph Font, Font: Not Bold, English
Figure 3),Figure 3), with an adjacent support, having a standard socket for holding a reflux condenser (United Kingdom)
(6.1.2.2)(6.1.2.2) with a graduated collector (6.1.2.3)(6.1.2.3) on one side.