Standard Test Method for Solvent and Fuel Resistance of Traffic Paint

SIGNIFICANCE AND USE
Traffic paints must have good resistance to motor oil and fuel drippings on the highway. This test method describes the procedure necessary to measure the resistance of traffic paint to reference test fluids in order to simulate this type of action.
SCOPE
1.1 This test method describes a laboratory test for determining the resistance of a dried film of traffic paint to the action of a specified hydrocarbon solvent or gasoline fuel test fluid.
1.2 The values stated in SI units are to be regarded as the standard. The values given in parentheses are for information only.
1.3 This standard does not purport to address all of the safety concerns, if any, associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and determine the applicability of regulatory limitations prior to use.

General Information

Status
Historical
Publication Date
30-Nov-2010
Current Stage
Ref Project

Relations

Buy Standard

Standard
ASTM D2792-69(2010) - Standard Test Method for Solvent and Fuel Resistance of Traffic Paint
English language
2 pages
sale 15% off
Preview
sale 15% off
Preview

Standards Content (Sample)


NOTICE: This standard has either been superseded and replaced by a new version or withdrawn.
Contact ASTM International (www.astm.org) for the latest information
Designation: D2792 − 69 (Reapproved2010)
Standard Test Method for
Solvent and Fuel Resistance of Traffic Paint
This standard is issued under the fixed designation D2792; the number immediately following the designation indicates the year of
original adoption or, in the case of revision, the year of last revision. A number in parentheses indicates the year of last reapproval. A
superscript epsilon (´) indicates an editorial change since the last revision or reapproval.
1. Scope procedure necessary to measure the resistance of traffic paint to
reference test fluids in order to simulate this type of action.
1.1 This test method describes a laboratory test for deter-
miningtheresistanceofadriedfilmoftrafficpainttotheaction
5. Apparatus
of a specified hydrocarbon solvent or gasoline fuel test fluid.
5.1 Tin Panel—Panels shall be cut from bright tin plate
1.2 The values stated in SI units are to be regarded as the
weighing not more than 25 g and not less than 19 g/dm (0.51
standard. The values given in parentheses are for information
to 0.39 lb/ft ). The panel should be about 75 by 130 mm (3 by
only.
5 in.).
1.3 This standard does not purport to address all of the
5.2 Film Applicator, which will producea3or 6-mil (76 or
safety concerns, if any, associated with its use. It is the
142-µm) (0.003 or 0.006-in.) wet film thickness.
responsibility of the user of this standard to establish appro-
6. Reagents and Materials
priate safety and health practices and determine the applica-
bility of regulatory limitations prior to use. 6.1 Test Liquid—The testing liquid shall be specified by the
purchaser and shall be selected from the following, dependent
2. Referenced Documents
on the paint tested:
6.1.1 Type I of Federal Specification TT-S-735 which is the
2.1 ASTM Standards:
same as ASTM Reference Fuel A (Test Method D471).
D471 Test Method for Rubber Property—Effect of Liquids
6.1.2 Type III of Federal Specification TT-S-735 which is
2.2 Federal Standard:
the same as ASTM Reference Fuel B (Test Method D471).
TT-S-735 Standard Test Fluids for Hydrocarbons
7. Procedure
3. Summary of Test Method
7.1 Clean the tin panels thoroughly with a suitable solvent,
3.1 The test paint is applied to a specified, properly
and buff lightly with fine steel wool. Prepare at least 3 panels
prepared, tin panel. After aging, the coated panel is immersed
for each paint to be tested.
in the hydrocarbon test fluid for a specified period of time at a
7.2 Examine the test paint, remove any skins that are
specified temperature. The paint is examined for blistering,
present, stir with a paddle to loosen any settled pigment, and
wrinkling, and loss of adhesion immediately upon removal and
mix thoroughly.
for complete hardness after a specified recovery time.
7.3 Draw down the material on the panels using a film
applicator that will produce a 76 or 142-µm (3 or 6-mil) wet
4. Significance and Use
film as specified by the purchaser.
4.1 Trafficpaintsmusthavegoodresistancetomotoroiland
7.4 Air dry the coating for the time specified by the
fuel drippings on the highway. This test method describes the
purchaser (usually 90 h) and then immerse the panels to half
their length in the test liquid contained in a covered glass
1 beaker at the temperature specified by the pu
...

Questions, Comments and Discussion